search  current discussion  categories  glazes - specific colors 

nickle yellow (fwd)

updated thu 16 dec 99

 

David Orser on wed 15 dec 99



---------- Forwarded message ----------
Date: Mon, 13 Dec 1999 03:08:58 -0500 (EST)
From: David Orser
To: JazNOTJazz@aol.com
Subject: nickle yellow


NICKLE YELLOW CONE 9-10 REDUCTION

CUSTER SPAR 32.58
F-4 SPAR 22.47
DOLOMITE 25.84
EPK 14.61
WHITING 4.49

ALSO:
TITANIUM DIOX 10.00
BLACK NICKLE OX 2.25

abeautiful and only slightly persnickity glaze. too thick & it will run.
nice on stone or porc. very yellow on porc. when thin.
microcrystalline, sugary matt. when medium thick and heavily reduced, will
form texured black outbursts. a very unique glaze. enjoy.

d.o. in ma and me.......