OOOPPPS< Forgot the recipe, Chris. here goes
Gerstley Borate 21.00 %
Neph Sy 16%
Kaolin 11%
Whititng 20%
Silica 32%

Also add:
Tin Ox 5%
Chrome Ox 0.15%