Y'all, please excuse me, as I am a total idiot. I went to look up my crawl
recipe to answer the request for Sperry Crawl and discovered MESSENGER'S
CRAWL in my glaze recipe file under "crawl." I fire this one to ^06, at
which temp Sperry's wouldn't work. So hope you didn't take my previous
advice. Duh. I know I used Sperry's when I was a college student, but
haven't a clue where I put it.

MESSENGER'S CRAWL ^04-06
borax 3.88
GB 46.51
Magnesium Carb 31.01
EPK 18.60
zircopax 5.43

Use over prefired dark glaze or ware. Subtle crawl, no craters on most
surface.


zahidi@gs.verio.net