glaze liner for woodfire

updated mon 13 sep 99

 

Wade Blocker on sun 12 sep 99

Dear Veena,

Here is a wonderful buttery glaze from Carlton Ball, Mg2 Matt cone
9 to l0

. It is an opaque waxy glaze

Soda spar 27
Ball clay 7.5
Gerstley borate ll.9
Dolomite 8.7
Talc l9.6
Flint 25.2

Mia in ABQ