I forgot who asked, but here the Sohngen Stony Yellow cone 10:


1675 Kona F4 Soda Spar
1250 Kaolin
850 Dolomite
525 Talc
350 Spodumene
225 Whiting
100 Bentonite
95 Red Iron Oxide

*For blue, lower Red Iron to 45 and add 45 cobalt carb

Regards,