Jeff Seefeldt on wed 23 jun 99

I did something tonight that I try not to do..I loaned out
my new magazine,, I think I will get it back, but we are
rakuing this weekend and I'd like to try a recipe that was
in there,, but I don't even know the last name of my class
mate that borrowed it.

Would someone please send the aqua blue raku glaze
recipe,,Please send it direct to me, so I can have time to
get some mixed up, and not have to wait for the messages to
get thu the list server..

thanks a bunch

jeff

weather here in Quincy IL is too humid for pots to dry, but
headed for the moutains ( denver ) over the 4th of July..

Jeff Seefeldt on wed 23 jun 99

Sorry I meant Clay Times,

jeff

Jeff Seefeldt wrote:

> I did something tonight that I try not to do..I loaned out
> my new magazine,, I think I will get it back, but we are
> rakuing this weekend and I'd like to try a recipe that was
> in there,, but I don't even know the last name of my class
> mate that borrowed it.
>
> Would someone please send the aqua blue raku glaze
> recipe,,Please send it direct to me, so I can have time to
> get some mixed up, and not have to wait for the messages to
> get thu the list server..
>
> thanks a bunch
>
> jeff
>
> weather here in Quincy IL is too humid for pots to dry, but
> headed for the moutains ( denver ) over the 4th of July..

Cheryl Fisher on thu 24 jun 99

Was it Erica's Aqua Cone 04 reduction/raku
furnished by Steve Branfman in the current issue of Clay Times

Gerstley Borate 80.00%
Cornwall Stone 20.00%
Total 100.00%

add: Tin Oxide 5.00%
Cobalt Carbonate 2.00%
Copper Carbonate 3.00%


--
Cheryl F.
cafish@gte.net
Sarasota, FL

Paul \"Standing Bear\" on thu 24 jun 99

Here is the glaze:

Erica's Aqua

Gerstley Borate 80%
Cornwall Stone 20@
Total--------------------------------
100.00%
then add: Tin Oxide 5.00%
Cobalt Carb. 2.00%
Copper Carb. 3.00%

Happy Rakuing! ^04

Paul
Inner Vision Earth Art
innervisionearthart@aol.com