ababy sharon on tue 16 feb 99

Well Brian I tryed it sometimes on different bases at 1100C And less(when my=
old
kiln-could=60nt climb above1060C It is hard to translat The frits .I If =
you have
a good base for=5E03 =5E04 you can add the Copper ox. 15=25is so much that =
it must
chang the glaze=21((Oxidatio))).
AnotherGaze...
Called Gold Bronze Igot from my teacher:At least 1100C-Oxidetion.

RedClay(Red Earth-is similar) 30
LEAD Frit 30
Silica 10
RIO 1(Maybe -not neededbecause thehigh
contents of the Red Clay)
Manganese 40
Copper Ox 10
And a local Clay Negev S-5:I canot Find It analisis. All Ican tell you is =
that
it comes from a beautifll place=21 You will have to try yourself to add the
=22other=22Clay.
And Raku with strong reduction.-Hop it helps-Ababi