I am trying to find a receipe for a raku glaze called Seth's
luster(matte)
Does this sound familiar to anyone?
TIA

Michelle

billie mitchell on sun 24 may 98

> ----------------------------Original message----------------------------
> I am trying to find a receipe for a raku glaze called Seth's
> luster(matte)
> Does this sound familiar to anyone?
> TIA
>
> Michelle
>
>i have the recipe for it. it has a sandy
texture. finally i have something to share
with someone. every one else has been so
good to share and ive learned alot.
seths luster
gerstly borate 4000.
bone ash 1000.
copper carbonate 500.
colbalt carbonate 250.
tin oxide 62.50
this is all in grams for us beginners
billie mitchell

billie mitchell on sun 24 may 98

> ----------------------------Original message----------------------------
> I am trying to find a receipe for a raku glaze called Seth's
> luster(matte)
> Does this sound familiar to anyone?
> TIA
>
> Michelle
>
>i forgot for those of you who dont know
what seths luster is its a racu glaze.
billie mitchell