Hello all,

I'm looking for a cone 5-6 oxidation glaze that gives a tan
finish with black specs. Kind of a salt fire/wood fire
look.

Any help would be greatly appreciated...

Thanks much,

John Baisch

David James on tue 10 mar 98

>----------------------------Original message----------------------------
>Hello all,
>
>I'm looking for a cone 5-6 oxidation glaze that gives a tan
>finish with black specs. Kind of a salt fire/wood fire
>look.
>
>Any help would be greatly appreciated...
>
>Thanks much,
>
>John Baisch


I use 33 percent calcined granite, 33 percent ball clay and 33 percent
hardwood ash to get mottled tan glaze that starts at cone 6

Dave James