cone 10 glossy green (hunter or so)...

updated sat 14 mar 98

 

Bob Hanlin on mon 9 mar 98

I need a cone 10R Hunter like green glaze. Anybody have one to share.


Bob Hanlin
bhanlin@ionet.net
Oklahoma City, OK

Maggie & David on thu 12 mar 98

Hello Bob, I don't know anything about this glaze but according to the
title, it might be worth a try. I'd be interested in your results. Maggie
in Mt. Shasta where it was actually warm today!


Deep Green ^10R

Kona F-4 feldspar 63.81
Flint 13.33
Gerst. Borate 8.57
Whiting 4.76
Bone Ash 4.76

Red Fe Ox 1.9
Cob. Ox .24
Chrome Ox .48
Maggie Shepard
FireWorks Pottery
Mt. Shasta, Calif.

Ron Roy on fri 13 mar 98

This looks like a durable glaze to me - it totals 97.85 and I wonder if I
have the whole story - but as it is "looking good."

I would feel better about using a glaze with the colouring oxides in
smaller amounts inside food containers. This is one of those glazes. It
will probably craze on porcelain but might be ok on some stoneware clays.

>----------------------------Original message----------------------------
>
>Deep Green ^10R
>
>Kona F-4 feldspar 63.81
>Flint 13.33
>Gerst. Borate 8.57
>Whiting 4.76
>Bone Ash 4.76
>
>Red Fe Ox 1.9
>Cob. Ox .24
>Chrome Ox .48
>Maggie Shepard
>FireWorks Pottery
>Mt. Shasta, Calif.

Ron Roy
93 Pegasus trail
Scarborough Otario
Canada M1G 3N8
Phone: 416-439-2621
Fax: 416-438-7849
Web page: Home page http://digitalfire.com/education/people/ronroy.htm