Maxine Peace Potter on mon 30 jul 12
The Tucson Clay Co-op is wondering what other potters are=3D0Ausing as subs=
ti=3D
tutes for primus and F4 feldspar and also what=3D0Aratios.=3DA0 If you are =
usin=3D
g Minspar as a substitute for=3D0AF4, let us know the ratio.=3D0A=3D0Amany =
thanks=3D
for your kind help=3D0A=3D0AMaxine
Steve Slatin on mon 30 jul 12
I have found Minspar to be a one-for-one substitute for=3D0AKona F-4.=3DA0 =
I ha=3D
ve never had Primus, so I can't speak to=3D0Ait.=3D0A=3D0ASteve Slatin -- =
=3D0A=3D0A=3D
=3D0AN48.0886450=3D0AW123.1420482=3D0A=3D0A=3D0A___________________________=
_____=3D0A=3D
=3DA0=3DA0=3D0A=3DA0 =3D0AThe Tucson Clay Co-op is wondering what other po=
tters are=3D
=3D0Ausing as substitutes for primus and F4 feldspar and also what=3D0Arati=
os.=3D
=3DA0 If you are using Minspar as a substitute for=3D0AF4, let us know the =
rati=3D
o.=3D0A=3D0Amany thanks for your kind help=3D0A=3D0AMaxine
James Freeman on mon 30 jul 12
Maxine...
I have been using NC4 feldspar from Zemex as a 1-1 substitute for F-4 for
about 5 or 6 years now, with no problems.
All the best.
...James
James Freeman
"Talk sense to a fool, and he calls you foolish."
-Euripides
http://www.jamesfreemanstudio.com
http://www.flickr.com/photos/jamesfreemanstudio/
http://www.jamesfreemanstudio.com/resources
On Mon, Jul 30, 2012 at 1:05 PM, Maxine Peace Potter <
maxinepeacepotter@yahoo.com> wrote:
> The Tucson Clay Co-op is wondering what other potters are
> using as substitutes for primus and F4 feldspar and also what
> ratios. If you are using Minspar as a substitute for
> F4, let us know the ratio.
>
> many thanks for your kind help
>
> Maxine
>
Julie Brooks on tue 31 jul 12
Hi All,
Got some info from production staff here
To sub for Primas P in glaze formulas use=3D20
50% G-200HP
50% Minspar=3D20=3D20
To sub for Primas S
100% Minspar
By the way, spelled Primas.
Thanks,
Julie Brooks
Creative Director, Laguna Clay Company
| |
|