wike on sun 18 jan 98

Could any of you describe any of the following 8 glazes in
terms of interest, gloss, shade of blue or whatever and whether
you have had good luck with it. Thank you so much. These came
off of Don's web page. Thank you Don for collecting these and
making them available. I downloaded the file and reformatted in
Word 7.0 so that I could fit them on 22 pages. If anyone wants
this Word document, I'll send it.
Patty
Wike@twave.net

BAY BLUE (^6 OX)

Gerstley Borate 5000
Ball Clay 1750
Flint 3250
Rutile 500
Cobalt Carb. 70
Cobalt Oxide 40
__________________________________
BLUE MATT (^6 OX)

Volcanic ash 55
Whiting 25
Baruim carb 10*
Ball clay 10 (I used OM#4)
Cobalt .5%
*CAN USE 7.5 of Stronium carb in place of the Barium
_________________________________________________________
BURGUNDY (^6 OX)

KONA FELDSPAR 53.00
SILICA 20.00
WHITING 15.00
BARIUM CARBONATE 6.00
EPK 6.00
add MASON DEEP CRIMSON STAIN 10.00
_________________________________________________________
DEEP BLUE (^6 OX)

Potash Feldspar 4400
Whiting 1700
Ball Clay 800
Kaolin 900
Flint 2200
Cobalt Oxide 500
Rutile 600
____________________________________________

DEEP SHINY BLUE (^6 OX)

Custer Feldspar 44
EPK 2
Colemanite 20
Whiting 4
Barium Carb 5
Flint 25
Copper Carb 6
Cobalt Oxide .9
Lithium Carb 4
_________________________________________
EMILY'S BLUE (^6OX)

Custer Feldspar 34
Gerstely Borate 18
Kentucky Ball Clay 10
Talc 14
Flint 10
Dolomite 6
Zircopax 4
Cobalt Carbonate 3
from Pam Glover pbg@po.cwru.edu
______________________________________
STALEY'S BLUE (^6 OX)

colemanite 2
whiting 15
custer spar 50
epk 13
flint 20
add
bentonite 2%
cobalt carb. 8%
red iron ox. 1%
____________________________________
VOLCANIC ASH BLUE MATT (^6 OX)

Volcanic ash 55
Whiting 25
Barium carb 10*
Ball clay 10 (I used OM#4)
Cobalt .5%
*CAN USE 7.5% STRONTIUM CARB