dj's perfect purple -- cone 6 gloss

updated thu 21 oct 10

 

DJ Brewer on wed 20 oct 10


Ilene Mahler asked about this purple glaze.

This purple is a cone 6

The firing ramp on this is probably important -- I have only fired this
once.

Here is the actual firing ramp

*ACTUAL FIRING RAMP */*note: kiln lid was cracked open for 14 hours of
firing. it was 1900 degrees when Jen closed it. My bad. Hence the ramp
was slowed to about 150 degrees per hour for 14 hours. Maybe more*/
*Ramp 1 -- 200 degrees an hour up to 2100 *
*Ramp 2 -- 100 degrees an hour up to 2232 -- hold 8 minutes*

*Ramp 3 -- drop at full speed to 1800*
*Ramp 4 -- 100 degrees an hour down to 1300
-- END OF FIRING --*


***
***

*DJ's PERFECT PURPLE CONE 6 (link is to picture. color is pretty accurate)
*http://2.bp.blogspot.com/_vBGPz8BmQTU/TLfS9cJOdqI/AAAAAAAABpY/KNgSPqsX-b8/=
s1600/1+PURPLE+GLAZE+SH105886.jpg

*cone 6*



*X1*



*X2*



*X3*



*X5*

*Neph Sy*



*18*



*36*



*54*



*90*

*Frit 3134*



*14*



*28*



*42*



*70*

*Whiting*



*20*



*40*



*60*



*100*

*OM4*



*18*



*36*



*54*



*90*

*Silica*



*30*



*60*



*90*



*150*

*total*



*100*



*200*



*300*



*500*

*oxides*













*Chrome Ox*



*0.2*



*0.4*



*0.6*



*1*

*Tin Ox*



*7.5*



*15*



*22.5*



*37.5*

*Cobalt Carb*



*1*



*2*



*3*



*5*

*RIO*



*0.5*



*1*



*1.5*



*2.5*




***
***




Here is the glaze recipe
*DJ's PERFECT PURPLE CONE 6*
*cone 6* *X1* *X2* *X3* *X5*
*Neph Sy* *18* *36* *54* *90*
*Frit 3134* *14* *28* *42* *70*
*Whiting* *20* *40* *60* *100*
*OM4* *18* *36* *54* *90*
*Silica* *30* *60* *90* *150*
*total* *100* *200* *300* *500*
*oxides* **
**
**
**
*Chrome Ox* *0.2* *0.4* *0.6* *1*
*Tin Ox* *7.5* *15* *22.5* *37.5*
*Cobalt Carb* *1* *2* *3* *5*
*RIO* *0.5* *1* *1.5* *2.5*