search  current discussion  categories  glazes - misc 

c/6 matt glaze

updated mon 23 nov 09

 

John Rodgers on sat 21 nov 09


What cone/temp

John Rodgers
Clayartist and Moldmaker
88'GL VW Bus Driver
Chelsea, AL
Http://www.moldhaus.com



Mike Gordon wrote:
> Sorry folks I forgot to include this info........ gas kiln, light
> reduction/oxidation atmosphere. From my previous entry. Mike Gordon
>
>

Mike Gordon on sat 21 nov 09


Sorry folks I forgot to include this info........ gas kiln, light
reduction/oxidation atmosphere. From my previous entry. Mike Gordon

Mike Gordon on sat 21 nov 09


Finally got to the studio & found this glaze. It's an old Albany glaze
that I have been playing with for a couple of years, off and on, more
off, since I fire so seldom. Buttery smooth slight crackle, at least on
flat tests.
400 grms Ravenscrag clay
300 grms Nepheline Syenite
300 grms Whiting
add 4% Rutile for a pale yellow.
Mike Gordon