Alisa Clausen on tue 16 sep 08


Recipe Name: Randy's 3 in one

Cone: Color:
Firing: Oxidation Surface: Glossy

Amount Ingredient
5 Gerstley Borate--1999
2 Whiting
41 Feldspar--Custer
12 Ball Clay--Old Mine #4
10 Red Art
6 Spodumene--Gwalia
11 Dolomite
7 Bone Ash
3 Talc
2 Lithium Carbonate
5 Silica

104 Total


Unity Oxide
.113 Li2O
.064 Na2O
.133 K2O
.229 MgO
.461 CaO
1.000 Total

.368 Al2O3
.049 B2O3
.016 Fe2O3

2.357 SiO2
.008 TiO2
.056 P2O5

6.4 Ratio
7.2 Exp
Comments: a semi gloss silk mat evenly covering glaze. Has a light tan
overall color. Smooth surface.
Because glaze is overall one color, does not give any breaking or layering
effect.