St. Johns Yellow (Not Food Safe - BARIUM)

Cone 9-10 in med to heavy reduction

Feldspar 1152
Whiting 12.8
Dolomite 409.6
Talc 83.2
Ball Clay 246.4
Flint 128
Ochre 9.6
Barium (TOXIC) 640
Zircopax 384
Iron 76.8
Bentonite 30 (at least)