glaze test for oil spot daly ^6 ox.

updated thu 5 jun 08

 

Alisa Clausen on wed 4 jun 08


Recipe Name: Oil Spot Daly

Cone: 6 Color:
Firing: Oxidation Surface: Oil Spot

Amount Ingredient
35 Feldspar--Custer
26 Silica
9 Whiting
9 Talc
9 Kaolin--EPK
15 Frit--Ferro 3195

103 Total

Additives
9 Iron Oxide--Red
2 Cobalt Carbonate

Unity Oxide
.12 Na2O
.139 K2O
.251 MgO
.49 CaO
1.000 Total

.405 Al2O3
.186 B2O3
.004 Fe2O3

4.063 SiO2
.001 TiO2
0 P2O5

10 Ratio
6.5 Exp
Comments: A blue ground with a brown shell, showing tea dust like spots
scattered overall.

Glaze test for Oil Spot, Daly ^6 ox.

Source: John Britt

Fired on mid fire white stoneware

Firing ramp with an electric controller is:
100c p/h to 600c (212f - 1112f)
150c p/h to 1140c (302f - 2084f)
80c p/h to 1220c (176f - 2228f)
15 min. soak
cool down max. to 900c (1652f)
Hold 30 minutes

Shut off kiln

Colorants or additives to a 100 gram batch are measured in percent to the
100 gram batch.
Standard Substitutions in all tests IF called for in recipe:
Local Boron Frit is used for Frit 3134
Forshammer (a half and half Potash and Soda spar) is the only Feldspar used
Local Boron Frit is used for Gerstley Borate