search  current discussion  categories  glazes - misc 

sagging glaze

updated tue 29 apr 08

 

Lee on sun 27 apr 08


Jeff,

Try this one:

*Phil Roger's Synthetic Nuka

Potspar 35.6
Whiting 21.8
Talc 2
Bone Ash 2
Ball Clay 5.9
Flint 29.7
ferro3134 3 (I have subbed wood ash)

add 4 to 5% for Seiji Green

Photo here:

http://public.fotki.com/togeika/pots_from_mashiko/aut_0020.html



--
Lee, a Mashiko potter in Minneapolis
http://mashikopots.blogspot.com/

"Not everything that counts can be counted, and not everything that
can be counted counts." --(Sign hanging in Einstein's office at
Princeton)

Jeff Gieringer on sun 27 apr 08


Hello,

I don't think this got through when Clayart went down. Sorry if it =
repeats. I'm looking for a ^10 glaze recipe that will move a little. Not =
necessarily run, but more like sag. I am using it as a top dip and =
would like it to sag down over the overlap. I have a gorgeous red and =
dark blue glaze I use, but they leave the dreaded straight line at the =
overlap. Thanks for any advice.

Jeff