Pat Walker on sat 18 aug 07


I'm looking for the recipe for June Perry's chrom red..I contacted her and
she told me to look on her web site under cone 6 glazes..I must be nuts but
I don't see that link ..I hate to bother her again. Anyone have the recipe
right off hand?

Dolita Dohrman on sat 18 aug 07


Here is the glaze site. I was able to access it using Safari on my
Mac but could not access it using Firefox. Strange.
Hope this helps!
http://www.angelfire.com/art2/shambhalapottery/c6glazegroup4.html
Dolita


On Aug 18, 2007, at 10:38 AM, Pat Walker wrote:

> I'm looking for the recipe for June Perry's chrom red..I contacted
> her and
> she told me to look on her web site under cone 6 glazes..I must be
> nuts but
> I don't see that link ..I hate to bother her again. Anyone have
> the recipe
> right off hand?
>

Charles on sat 18 aug 07


http://www.angelfire.com/art2/shambhalapottery/c6glazegroup4.html=0A =0A=0A=
Visit me on the web www.hughespottery.com=0A=0AInterested in lessons? www.t=
hecreativeoasis.com=0A=0A=0A =0A=0A=0A=0A----- Original Message ----=0AFrom=
: Pat Walker =0ATo: CLAYART@LSV.CERAMICS.ORG=0ASent:=
Saturday, August 18, 2007 10:38:44 AM=0ASubject: [CLAYART] chrom red glaze=
(June Perry's)=0A=0AI'm looking for the recipe for June Perry's chrom red.=
.I contacted her and=0Ashe told me to look on her web site under cone 6 gla=
zes..I must be nuts but=0AI don't see that link ..I hate to bother her agai=
n. Anyone have the recipe=0Aright off hand?=0A=0A_________________________=
_____________________________________________________=0ASend postings to cl=
ayart@lsv.ceramics.org=0A=0AYou may look at the archives for the list or ch=
ange your subscription=0Asettings from http://www.ceramics.org/clayart/=0A=
=0AModerator of the list is Mel Jacobson who may be reached at melpots@pcli=
nk.com.=0A=0A=0A

Maurice Weitman on sat 18 aug 07


At 09:38 -0500 on 8/18/07, Pat Walker wrote:
>I'm looking for the recipe for June Perry's chrom red..I contacted her and
>she told me to look on her web site under cone 6 glazes..I must be nuts but
>I don't see that link ..I hate to bother her again. Anyone have the recipe
>right off hand?

Yes, and so do you, Pat.

Searching the archives, or Google, would reveal all.

June's site is a bit under the weather... she's in the process of
redoing it and links aren't working well.

The glaze June had there is actually Lana Wilson's.

Here's a reference to it in the archives:

Ann Stecker on tue 12 jan 99

Here is the Chrome Red glaze from Lana Wilson's book. Several people
have contacted me asking for it so I thought there may be others
interested.

Chrome Red ^6

Gerstley Borate 21
Neph Sy 16
Kaolin 11
Whiting 20
Silica 32
Tin 5
Chrome .15

Regards,
Maurice, in Fairfax, California, where I'm wondering whether people
with pissy rants about misspellings will expect me to correct
spellings on others' posts.