My apologies for not including the cone number.

It is cone six oxidation and a very nice glaze.

Here is the recipe again.

Flint 29
Calcium carb 13
Frit 3134 19
kona F4 20
Kaolin - pioneer 19

Superpax 12.5


Art Powell
Black Bear Pottery,
Kitamaat Village,
British Columbia