search  current discussion  categories  techniques - slips 

universal slip rec.

updated fri 31 may 96

 

p4337@freenet.edmonton.ab.ca on mon 20 may 96

Hi all...those asking for the universal slip rec...follows.

Basic White Slip ~04 to ~12
Ball Clay 75 grms
Kaolin 10
Flint 10
Feldspar 5
Total....100
This slpi is excellent with mocha diffusion and all other slip
appications. Color as desired...oxides and stains. The wet mix is rather
a gray color but fires very white.
As Always in Clay Peggy

Peggy Heer/Heer Pottery E-Mail: p4337@freenet.edmonton.ab.ca
9702-76 Ave Edmonton,AB *OR* e-mail: p4337@connect.ab.ca
CANADA T6E 1K3 http://www.ffa.ucalgary.ca/artists/pheer/
PH: (403) 433-0290
--------------------------------------------------------------------

Donald Goldsobel on tue 21 may 96

>----------------------------Original message----------------------------
>Hi all...those asking for the universal slip rec...follows.
>
>-------------------------------------------------------------------->Peggy
is this universal slip for bisque ware, grenware, wet ware etc?


Donald Goldsobel
>

p4337@freenet.edmonton.ab.ca on thu 23 may 96

Hi Don...the slip is for wet OR greenware.
It is made with a lot of clay so needs to go on wet clay to stick. Color
it and it is great. from ^04-^12 Oxidation/electric or reduction.
As Always in Clay Peggy
--------------------------------------------------------------------
On Tue, 21 May 1996, Donald Goldsobel wrote:

> ----------------------------Original message----------------------------
> >----------------------------Original message----------------------------
> >Hi all...those asking for the universal slip rec...follows.
> >
> >-------------------------------------------------------------------->Peggy
> is this universal slip for bisque ware, grenware, wet ware etc?
> Donald Goldsobel
> >
>

Peggy Heer/Heer Pottery E-Mail: p4337@freenet.edmonton.ab.ca
9702-76 Ave Edmonton,AB *OR* e-mail: p4337@connect.ab.ca
CANADA T6E 1K3 http://www.ffa.ucalgary.ca/artists/pheer/
PH: (403) 433-0290
----------------------------------------------------------------