search  current discussion  categories  glazes - traditional iron glazes 

tessha

updated sun 31 aug 97

 

Poseyb@aol.com on sat 2 aug 97

Steve
I have the folowing recipe for Tessha. It is the one used by Michael Simon.
He uses it in salt firing and it comes out a beautiful yellow. I think in
reduction it is different.

Tessha
Ball Clay 1626
Silica 1626
Potash Spar 1500
Whiting 1080
Red Iron Oxide 660

Hope this helps
Posey