SUSAN DEMAY CONE 6 GLAZES

A. GLAZE RECIPES COLLECTED FROM VARIOUS SOURCES:

PEACHY KEEN KEEN GREEN

Gerstley Borate 1224 Gerstley Borate 1088
Potash Feldspar 4140 Potash Feldspar 3680
Flint 1692 Flint 1504
Kaolin 225 Kaolin 200
Whiting 729 Whiting 648
Zircopax 540 Zircopax 480
Dolomite 540 Dolomite 480
Bentonite 90 Bentonite 80
Rutile 720 Rutile 200
7% Copper Carb. 571.2

TRANSPARENT CONE 6 BLACK MIX

Potash Feldspar 3960 Cobalt Oxide 310
Zinc Oxide 450 Chrome Oxide 70
Gerstley Borate 1710 Red Iron Oxide 370
Dolomite 540 Manganese Dioxide 120
Whiting 180 Nickel Oxide (green) 130
Kaolin 450
Flint 1710
*Black Mix 630

MY GREEN BAY BLUE

Potash Feldspar 5280 Gerstley Borate 5000
Zinc Oxide 600 Ball Clay 1750
Gerstley Borate 2280 Flint 3250
Dolomite 720 Rutile 500
Whiting 240 Cobalt Carb. 70
Kaolin 600 Cobalt Oxide 40
Flint 2280
Copper Carb. 360
Red Iron Oxide 240
Rutile 360

SANDY LIGHT YELLOW

Gerstley Borate 1470 Potash Spar. 606
Kaolin 510 Flint 402
Flint 1020 Gerstley Borate 402
Zircopax 45 Kaolin 204
Yellow Stain 15 Dolomite 200
Yellow Stain(6485 Titanium) 102
Tin Oxide 60


DEEP BLUE KLINESVILLE GOLD

Potash Feldspar 4400 Magnesium Carb. 359.2
Whiting 1700 Whiting 1618.4
Ball Clay 800 Wollastonite 449.6
Kaolin 900 Neph Sy. 4494.4
Flint 2200 Cedar Hts. Red Art 1078.4
Cobalt Oxide 500 Red Iron Oxide 539.2
Rutile 600 Zircopax 988.8


CONE 6 CASTING SLIP

Custer Feldspar 4000
Gold Art Clay 3000
Red Art Clay 1000
Kaolin 5800
Ball Clay 3000
Flint 3200
Darvan 7 140 Suggestion: for easy weighing of the darvan,
Water 10,000 add to the last 500 grams of water.


B. SLOP/SCRAP GLAZE MIXTURES:
The basic ingredient for the Mystery Glazes is the sedimet from
the glaze table wash-off buckets. Allow the buckets to settle
overnight. Carefully decant all the water off the top of the bucket
and mix the remaining sediment thoroughly. Test batches of 1,000 gr.
of the sediment are mixed with colorants at 1% to 10% and test tiles
are fired. Here are some of my Mystery Glazes. These batches are for
about 5 gal.

MYSTERY BLUE FLORENTINE GREEN

23,000 gr. base 23,000 gr. base
81 gr. Cobalt Carbonate 1,150 gr. Mason Florentine Green

MAZERINE BLUE

23,000 gr. base
920 gr. Mason Mazerine Blue


C. BURGANDY, GRAPE, PINK---COMMERCIAL GLAZES SUCH AS OPULENCE GLAZE.