search  current discussion  categories  glazes - cone 4-7 

pearly ^6

updated wed 30 apr 97

 

Steve Williams on mon 28 apr 97

Hi Folks!

Here's a glaze I've been meaning to send for a while.

Pearly ^6

K200 Feldspar 26.3
Flint 32.69
Whiting 19.72
EPK 12.05
Zinc 6.57
Magnesium
Carbonate(light) 2.66
----
100

Additions:
rutile 10% Glossy pearly white to orange with yellow highlights where
thick. Best when applied thickly. Be careful it might run some.

Steve Williams
sawilliams@skybest.com

Julia Townsend on tue 29 apr 97

Oxidation or Reduction??

Steve Williams wrote:
>
> ----------------------------Original message----------------------------
> Hi Folks!
>
> Here's a glaze I've been meaning to send for a while.
>
> Pearly ^6
>
> K200 Feldspar 26.3
> Flint 32.69
> Whiting 19.72
> EPK 12.05
> Zinc 6.57
> Magnesium
> Carbonate(light) 2.66
> ----
> 100
>
> Additions:
> rutile 10% Glossy pearly white to orange with yellow highlights where
> thick. Best when applied thickly. Be careful it might run some.
>
> Steve Williams
> sawilliams@skybest.com