paul davis' shino

updated fri 31 may 96

 

tony nankervis on wed 8 may 96

Somebody recently posted a recipe for this glaze. I don't seem to be able
to search the archives - does anyone still have the recipe - thanks

Tony Nankervis
Ceramics Dept
Visual Arts
Southern Cross University
Lismore 2480 NSW Australia

KEMPB on thu 9 may 96

From one Oz to another,
The Paul Davis Shino recipe I have is:
Nepheline Syenite 47.6, Spodumene 31.8, Zirconium Silicate 4.8, Alumina
Hydrate 12, Salt 2, Bentonite 4
Brian Kemp. Singapore