glazes we use, continued

updated tue 31 dec 96

 

Samantha Tomich on tue 10 dec 96

Spodumene


Custer spar 30
EPK 25
Dolomite 22
Spodumene 20
Whiting 3
Superpax 10
Bentonite 2


recipe says cone 9, but we often get up to cone 11 and have had no
trouble.
smooth surface, not shiny, not dry, nice matte tan and white




Oatmeal

Custer spar 31.5
Colemanite 28.1
EPK 20
Talc 16.8
Superpax 15.5
Lithium .68
Red iron oxide 1
Bentonite 2



recipe says cone 5-10, but we've never fired below 9
slightly glossy, tan w/brown specks


Samantha Tomich
Paauilo, Hawaii