glazechem - eucalptus???

updated fri 31 jan 97

 

Numo Jaeger and Michael Miller on sat 25 jan 97

Hi Folks,
Does anyone have the approximate analysis for Eucalptus?

Numo Jaeger
Studio One Art Center
365 45th Street
Oakland, CA 94602

e-mail:jaegmil@ccnet.com

At 06:50 AM 1/24/97 EST, you wrote:
>----------------------------Original message----------------------------
>Date: Wed, 22 Jan 1997 09:11:55 EST
>John Weber wrote:
>>> I would appreciate anyone who has a "theoretical" formula for Hardwood Ash
>that could be used in the GlazeChem software so I can get at least an
>approximate analysis. <<
>
>The following analyses are taken from Phil Rogers' book _Ash Glazes_:
>
>APPLE
>----------
>SiO2 1.31
>Al2O3 -
>P2O5 4.9
>Fe2O3 1.66
>CaO 63.6
>K2O 19.24
>MgO 7.46
>Na2O 10.45
>MnO -
>SO3 0.93
>CuO -
>Cl 0.45
>
>BEECH
>-----------
>SiO2 3.01
>Al2O3 -
>P2O5 6.2
>Fe2O3 0.62
>CaO 42.00
>K2O 24.29
>MgO 8.20
>Na2O 8.34
>MnO 4.52
>SO3 2.10
>CuO -
>Cl 0.72
>
>OAK
>--------
>SiO2 15.30
>Al2O3 0.13
>P2O5 13.8
>Fe2O3 2.40
>CaO 30.02
>K2O 14.00
>MgO 12.01
>Na2O 9.12
>MnO 0.10
>SO3 2.61
>CuO 0.05
>Cl 1.18
>
>PINE
>--------
>SiO2 10.00
>Al2O3 0.43
>P2O5 8.8
>Fe2O3 4.00
>CaO 25.00
>K2O 26.50
>MgO 6.32
>Na2O 8.65
>MnO 5.06
>SO3 4.63
>CuO
>Cl 0.52
>
>SPRUCE
>-------------
>SiO2 2.73
>Al2O3 -
>P2O5 2.12
>Fe2O3 1.42
>CaO 33.97
>K2O 19.66
>MgO 11.27
>Na2O 1.37
>MnO 22.96
>SO3 2.64
>CuO -
>Cl 0.07
>
>WILLOW
>-------------
>SiO2 4.44
>Al2O3 0.05
>P2O5 10.00
>Fe2O3 1.25
>CaO 20.21
>K2O 49.8
>MgO 8.26
>Na2O 2.50
>MnO 0.18
>SO3 1.22
>CuO -
>Cl 0.08
>
>- Bill Amsterlaw (wamster@msn.com)
> Plattsburgh, NY
>
>

gail@matra.com.au on sun 26 jan 97

>----------------------------Original message----------------------------
>Hi Folks,
>Does anyone have the approximate analysis for Eucalptus?

This analysis is one of many given in Notes for Potters in Australia, by
Ivan McMeekin:

Average of 10 analyses of New South Wales (Australia) eucalypts:
SiO2 30.1
Al2O3 2.1
Fe2O3 2.6
MgO 13.3
CaO 21.7
Na2O 10.4
K2O 10.8
MnO 0.6
P2O5 3.8
SO3 4.0

I don't know if the book is available in the USA. It's published by the New
South Wales University Press.
..............................................................
Gail Nichols gail@matra.com.au
SODA GLAZE CERAMICS http://www.matra.com.au/~gail/
Sydney, Australia
..............................................................