search  current discussion  categories  glazes - misc 

fw: funky glazes, revisited or saving ralph's hide!

updated thu 31 oct 96

 

RALPH on tue 8 oct 96



----------
From: Susan Maguire[SMTP:smaguire@bcfreenet.seflin.lib.fl.us]
Sent: Monday, October 07, 1996 07:51
To: RALPH
Subject: Re: Funky Glazes, revisited or saving Ralph's hide!

>>>My wife has threatened me with dire
circumstances
> if I do not get them. We had them and tested them all. A few of them she
> absolutely adores. So could somebody please save my hide.<<<<

Hi all.... These were some Cone 06 - 04 glazes that I had posted
last year... Now seems as tho a few people want them again. So just because
I like you-all so much, here goes again!

Lichens:
50 Magnesium Carbonate
10 Lithium Carbonate
50 Borax
30 Gerstley Borate
4 Copper Carbonate
0.4 cobalt carb

Lizard:
40 Magnesium Carb
15 Lithium Carb.
10 Borax
70 Gerstley Borate
5 Silica
20 Neph. Syenite
0.4 Chrome Oxide

Craters:
20 Magnesium Carb
20 Kaolin
60 Lithium Carb.
30 Borax
12 Copper Carb.
60 Silica
10 Bentonite

Earthmother:
30 Lithium Carb
30 Gerstley Borate
3 Copper Carb.
20 Silica
1 Cobalt Carb.
10 Ball Clay
10 Talc
3 Manganese dioxide

Ocean Oil:
10 Kaolin
30 Lithium Carb.
20 Borax
40 Gerstley Borate
6 Copper Carb
40 Whiting

Superstition:
30 Lithium Carb.
40 Gerstley Borate
3 Copper Carb.
0.5 Cobalt oxide
30 Talc
10 Neph. Syenite

Beads:
50 Magnesium Carb.
40 Borax
50 Gerstley Borate
10 Silica
10 Zircopax

Please test as these certainly are FUNKY!!!!