Greg Lamont on sun 26 oct 97

Liz and all Clayarters,

Bill Amsterlaw brought it to my attention that a typo occured in my recent
posting of the following glaze recipe.
The Percentage of Gerstley Borate should have read 20.68 and NOT .68
percent. The corrected version appears below:

Glaze name: Pink? Glaze
Cone: 4 - 5 - 6
Color: semi-opaque pink
Testing: Tested
Surface texture: shiny
Firing: Oxidation
Glaze type: Ca B

Recipe: Percent Batch
Gerstley Borate 20.68 1034
Nepheline Sye. 16.29 814
EPK 11.34 567
Whiting 19.52 976
Flint 32.16 1608
Totals: 100.00 % 5000 gm

add: 12% Deep Crimson Mason Stain, or .15% Green Chrome Oxide and 5% Tin
Oxide

My sincere apologies for any inconvenience this may have caused.