charcoal briquette ash glaze

updated sat 31 aug 96

 

June Perry on thu 1 aug 96

Here is the recipe for the briquette ash glaze:

Doug's Honey Cone 10 R.

35 Custer Feldspar
35 Briquette ash (unwashed)
15 E.P.K.
15 Dolomite

Add: 5% Zircopax


June Perry