c/9 green glaze

updated fri 24 oct 97

 

Dana Henson on mon 20 oct 97

Jack McCoy,
A glaze recipe that I personally tested as an undergraduate clay student
was "Hamada Green." This is a good strong, deep green and does not contain
chrome. We fired to c/10 reduction but you might try this glaze at c/9.
-----HAMADA GREEN-----
Custer Feldspar 53
Barium Carbonate 21
Whiting 9
Zinc Oxide 9
OM4 Ball clay 1
Rutile 2
Copper Carbonate 3
Red Iron Oxide 2.5
Bentonite 2
_______
102.5