search  current discussion  categories  glazes - cone 4-7 

^6 stoneware ox. give this a shot.

updated tue 30 sep 97

 

Kevin F. King on sun 21 sep 97

Here's a little something I came across while cleaning out my glaze
notebook. Fires to a nice deep burnt red in oxidation on buff stoneware.

EPK 5
Flint 30
Custer 25
Talc 15
Gerstley Borate 25
add:
Red Iron 15

Give it a shot, let me know what you think,
Kevin King
kingx61@ibm.net