^6 clay body larry bush rev. jason stone iii

updated thu 31 oct 96

 

Omer.Artun@cns.brown.edu on thu 10 oct 96


A lot of people asked me about the clay body I use for
Rust red and Celadon. Here it is,

I



risd96 (Jason STONE III revised by Larry Bush-- my mentor)

ocmulgee 14.87
goldart 14.19
redart 13.51
xx sagger 12.84
flint 12.16
om4 11.49
custer 10.81
Tile #6 10.13
-----
100.00

+ bentonite 3.00
+ epsom salt small hand full



this is a cone 6 high iron (2.5% RIO) that it bleeds through a little,
it is a warm
brown thermal shock resistant , good for both throwing and handbuilding

--
-----------------------------------------------------------------------------